[TheForge] Super Quenched Dies?

schade at acegroup.cc schade at acegroup.cc
Wed Apr 20 09:32:43 EDT 2005


On Apr 20, 2005, at 7:20 AM, Ron Childers wrote:

> Echo Dan: *Don't*
>
>


Why not?

Dave Mudge reported that he has been using unhardened 4140 for a period 
of time with no wear. Surely the superquenched dies would be as hard as 
unhardened 4140.

If you are worried about the superquenched dies being too hard due to 
unknown carbon content use 1018.

I say go for it Carl. 1018 is readily available, cheap and easy to work 
with.

Here is what Dave Brown had to say about Superquench...

Bob
__________

> http://www.lametalsmiths.org/news/robb_gunter.htm

>
> Whether its on the internet group "theforge", at ABANA chapter 
> conferences, or just general discussion between a couple of friendly 
> smiths, when the subject of Robb Gunter's "Super Quench" comes up, 
> most of it is fact, but some of what is passed around is erroneous. 
> Yes, there are some errors, but generally minor. There is often a 
> great deal of disbelief as to the efficacy of this Super Quench. 
> Here's what he had to say about it at the Guild of Metalsmiths 1997 
> Fall Conference: 
>
> Before the Bessemer process made it feasible to effectively control 
> the amount of carbon in steel, blacksmiths generally had only iron or 
> tool steel to work with. The Bessemer process gave the steel 
> manufacturers the ability to produce steel in a variety of carbon 
> levels. Mild steel (1005, 1018, and the like) was touted as the all 
> purpose steel destined to replace wrought iron. The manufacturers 
> claimed that it was also suitable for many tools, but that it should 
> be quenched in a solution of sodium hydroxide. 
>
> At Sandia Labs, Robb and his cohorts experimented with this lye quench 
> and, a bit to their surprise, they found that mild steel hardened 
> considerably more that expected. Metallurgists and others will tell 
> you quite readily that mild steel won't harden. It may get a little 
> harder than if annealed, however it doesn't harden in the typical 
> toolmaker's sense of hardening. Generally speaking, in a plain water 
> quench you shouldn't expect to get more than Rockwell ratings in the 
> low to mid 30's. Robb found that the sodium hydroxide quench resulted 
> in average Rockwell ratings in the 43-45 range, with an occasional 
> test result as high as 48. 
>
> So, Robb started using this solution at Sandia Labs, but installed a 
> vented hood system over the quench tank. This stuff is pretty harsh 
> and the need for a vented hood was a no-brainer.
>
> Then OSHA arrived on the scene and insisted that the use of the sodium 
> hydroxide solution cease. The result was that Robb and the Sandia Labs 
> metallurgical lab crew went to work to find a replacement solution. It 
> had to give hardness results comparable to the sodium hydroxide 
> solution, and it should be bio-degradable if possible. The result of 
> their experimentation was what is now generally referred to as 
> Gunter's Super Quench. The formulation is as follows: 
> 	• 	5 gallons of water (This a good volume to work with for quenching, 
> and there are plenty of buckets and pails around just the right 
> size.) 
>
>  
> 	• 	5 lbs table salt (plain or iodized, canning salt or rock salt, it 
> makes no difference.) 
>
>  
> 	• 	32 oz Dawn Liquid Dishwashing Detergent (blue. Blue was chosen 
> because that's what happened to be available at the moment. It was 
> noted later on that as the solution deteriorated to the point that it 
> should be disposed of, the color slowly changed to green. Hence, the 
> blue detergent is recommended. Any other blue colored liquid detergent 
> could work just as good.) 
>
>  
> 	• 	8 oz Shaklee Basic I. (The solution needs a surfactant to maximize 
> contact between the solution and the piece being quenched. Amway Basic 
> H will also work. Your local farmer's supply should be able to help 
> here, as similar surfactants are used to facilitate the distribution 
> of fertilizer in soil. In response to a question from the viewing 
> stands, Robb said that just about any wetting agent should do, even 
> the stuff photo film developers use. Just follow directions on amount 
> of agent to be added to a given amount of water, then scale up or down 
> to the 5 gallons of water used in this formulation.) 
>
> Heat your iron to 1550 degrees Fahrenheit, and quench. No tempering is 
> needed. 
>
> So, he mixed up a batch right there in front of us and used it for his 
> next demonstration. He took a piece of 1/2" 1018 and cut off a piece 
> about 3" long. This piece was heated in the gas forge, and a cold 
> chisel end was forged on to it. Robb heated the piece to 1550 
> (critical temp for mild steel), and quenched it in the solution. He 
> then took his new "chisel" and proceeded to use it to cut almost 
> through the parent bar. Then, he did it again. The cut bar and the 
> chisel were passed around for all to take a good look at. The edge on 
> the chisel was not deformed in any way. The top had not mushroomed, 
> nor did it even show any evidence of having been hit with the hammer. 
> But, so as not to mislead us, Robb said that a chisel of this type 
> might be good for 7 or 8 cuts maximum. He recommends this quench for 
> tools such as spring fullers and many treadle hammer 
> tools/dies/fullers. He showed, and used, one such spring fuller that 
> is made of mild steel and quenched in the solution. He has been using 
> this particular fuller for several years with no ill effect. The 
> fuller is unmarred, and the spring is still strong. 
>
> I was impressed, to say the least. I was not the only person there who 
> was "wowed" by this little "trick". Robb said the quench is good for 
> anything up to 50 points of carbon. Above this carbon level this 
> quench should not be used. 
>
> The above is how I heard it from Robb Gunter at the Guild of 
> Metalsmiths 1997 Fall Conference.  
>
> Dave Brown
>  Heritage 'Smithing
>  Heritage Hill State Historical Park
>  Green Bay, WI  
>
>
>  


More information about the TheForge mailing list