250 degrees in the oven should do it for a couple of hours.
Ray Miller
Cincinnati
>
> From: "irontree" <[email protected]>
> Date: 2003/08/07 Thu PM 02:56:39 EDT
> To: <[email protected]>
> Subject: Re: [TheForge] Stick welding question
>
> Thanks...I got a box (20 lbs) of free rods (6013) from a school metal shop
> that was closing. The rod was really old and sitting in a cardboard box in
> a closet for years. I am betting humidity unless flux can spoil??? I'll
> try baking them for a bit
>
> Temperature? time? Can I just put them on a stainless steel broiler
> pan?....Will it ruin the pan?
>
> Dan
> -----Original Message-----
> From: Ralph Sproul <[email protected]>
> To: [email protected] <[email protected]>
> Date: Thursday, August 07, 2003 12:32 PM
> Subject: Re: [TheForge] Stick welding question
>
>
> >Dan, It sounds like if you have the same welder, on the same amperage,
> >using the same rods, it is a humidity problem with all the rain and humid
> >weather we've had lately. If the flux is blistering off when you strike
> and
> >arc that is definitly the problem - but that's usually when it's real bad.
> >
> >Ralph
> >----- Original Message -----
> >From: "irontree" <[email protected]>
> >To: <[email protected]>
> >Sent: Thursday, August 07, 2003 10:15 AM
> >Subject: [TheForge] Stick welding question
> >
> >
> >> Hey all,
> >>
> >> I need some welding advice.
> >>
> >> I have an old Lincoln buzz box (220 volts, 50 amps). Lately my welds
> have
> >> been filled with bubbles. What's wrong?
> >>
> >> possiblilties: Old sticks?, too much amperage?, sticks left sitting out
> >> (humidity)?, etc.
> >>
> >> Any advice?
> >>
> >> Dan
> >> www.irontreeworks.com
> >>
> >>
> >>
> >> _______________________________________________
> >> http://mailman.qth.net/mailman/listinfo/theforge
> >> theforge mail list group photo site is
> >> http://www.photoaccess.com
> >> Login: [email protected]
> >> password: anvil
> >> ___________
> >>
> >>
> >
> >_______________________________________________
> >http://mailman.qth.net/mailman/listinfo/theforge
> >theforge mail list group photo site is
> >http://www.photoaccess.com
> >Login: [email protected]
> >password: anvil
> >___________
> >
> >
>
>
> _______________________________________________
> http://mailman.qth.net/mailman/listinfo/theforge
> theforge mail list group photo site is
> http://www.photoaccess.com
> Login: [email protected]
> password: anvil
> ___________
>
>
>