Peter,
Bare wire Mig is DC reverse polarity (positive electrode), flux core is
strait polarity. 75/25 mix is ideal, all positions. Some good info here:
http://www.welding-advisers.com/Mig-welding-tips.html
Good luck
Peter Fels & Phoebe Palmer wrote:
> Been trying to figure out MIG spray deposition now that i have the power
> to do it.
> Using .035 wire and argon75% CO2 25% mix gas. Electrode negative.
> If i crank it up to about 400 ipm and about 25 volts i get spray
> deposition as i imagine it to be, but the nozzle and contact tip seem to
> foul pretty quickly.
> Part of the problem was the awkward position of the welds and a sore
> back...which contributed to the fouling i'm sure.
> Looking on the web, they were talking about a different gas mix ( i was
> using what i have and can easily get) and electrode positive setting.
> Is that right? I keep imagining the wire fusing to the contact tip as
> soon as the trigger is pulled with electrode pos.
> Can the gas i have be made to do spray deposition decently?
> Sure appreciate having you folks around to straighten my path every now
> and then...pete f
> ______________________________________________________________
> TheForge mailing list
> Home: http://mailman.qth.net/mailman/listinfo/theforge
> Help: http://mailman.qth.net/mmfaq.htm
> Post: mailto:TheForge at mailman.qth.net
>
> This list hosted by: http://www.qsl.net
> Please help support this email list: http://www.qsl.net/donate.html
>
>
More information about the TheForge
mailing list