[TheForge] oxy-propane torch equipment
terry l. ridder
terrylr at blauedonau.com
Sun Aug 15 14:20:48 EDT 2004
hello;
as a follow-up to my previous reply i found my oxy-fuel comparison
chart:
Table : Fuel Gas Characteristics
Fuel Gas Maximum Flame Oxygen to fuel gas Heat distribution
Temperature °C Ratio (vol) kJ/m3
Primary Secondary
Acetylene 3,160 1:5 18,890 35,882
Propane 2,810 4.3:1 10,433 85,325
MAPP 2,927 3.3:1 15,445 56,431
Propylene 2,872 3.7:1 16,000 72,000
Hydrogen 2,834 0.42:1 - -
Natural Gas 2,770 1.8:1 1,490 35,770
as the above chart shows, oxygen use is going to increase 4.3 times when
using propane instead of acetylene.
fuel gas flame speed
acetylene 7.4m/s
propane 3.3m/s
mapp 4.69m/s
hydrogen 14.35m/s
natural gas 3.9m/s
On Sat, 14 Aug 2004, John Switzer wrote:
john>
john> I am in the middle of a project using a torch to archive a local heat for
john> an upset on 1" bars. Using oxy-acetylene is getting pretty expensive (an
john> acetylene bottle lasts about 20 upset bars) I was wondering about
john> switching to oxy-propane. Does anyone know what additional equipment would
john> be required, besides a propane rosebud tip. Is it OK to just move my
john> existing acetylene regulator back and forth as the need changes?
john>
john> Thanks
john>
john> John Switzer
john>
--
terry l. ridder ><>