>#1 - Cracked pan. 
>The pan has a crack 3/4 of the way across the bottom. Since I am planning on
>lining the pan with clay, I don't think the crack will be a problem. Am I
>wrong? 
 

I RECENTLY WELDED UP A CAST PAN WITH A MIG SETUP USING STAINLESS WIRE (ER308L).030, IT HAS PLENTY OF Ni AND DOESNT HEAT IT UP AS MUCH AS STICK AND BRAZING. BEWARE OF THE DREADFUL "PING".
1" INTERMITTENT WELDS, LET COOL BEETWEEN EACH STITCH, IT IS RATHER TIME CONSUMING, BUT MOST EFFECTIVE. IT HAS TO BE CLEANED WELL.


---------------------------------------------