Hi Al;
I've the same frustrations but mostly cause i feel compelled to get in that one last whack.
The trick, i've found, is acoustical. When the bronze starts to tighten up, the hammer fall sound will change from
a meaty "thud" towards a higher frequency . You want to stop hitting it during that transition.
By the time it sounds like you are hitting something hard, you are asking for cracking.
On Feb 18, 2013, at 9:56 AM, aavasaris at comcast.net wrote:
I have forged bronze successfully for the past couple of years. In my opinion, silicon bronze is the best for forging. It is also sold under the "Everdur" designation. I bought mine from Atlas. Aluminum bronze forges more like steel, but still workable under a hammer. Other unidentified bronzes that I have tried have not worked well. They tend to crack on their way down from optimum forging temperature. Very frustrating trying to judge when that is.
Al Vasaris
Jackson, MI
----- Original Message -----
From: theforge-request at mailman.qth.net
To: theforge at mailman.qth.net
Sent: Monday, February 18, 2013 12:00:04 PM
Subject: TheForge Digest, Vol 109, Issue 17
Send TheForge mailing list submissions to
theforge at mailman.qth.net
To subscribe or unsubscribe via the World Wide Web, visit
http://mailman.qth.net/mailman/listinfo/theforge
or, via email, send a message with subject or body 'help' to
theforge-request at mailman.qth.net
You can reach the person managing the list at
theforge-owner at mailman.qth.net
When replying, please edit your Subject line so it is more specific
than "Re: Contents of TheForge digest..."
Today's Topics:
1. Re: looking for"real" bronze (Peter Fels & Phoebe Palmer)
----------------------------------------------------------------------
Message: 1
Date: Sun, 17 Feb 2013 21:30:13 -0800
From: Peter Fels & Phoebe Palmer <artgawk at thegrid.net>
To: Blacksmithing List Sponsored by ABANA <theforge at mailman.qth.net>
Subject: Re: [TheForge] looking for"real" bronze
Message-ID: <5D059F20-AAC2-479D-B393-A12FEFE93AA9 at thegrid.net>
Content-Type: text/plain; charset=us-ascii
Acknowledging that my alloy ID is often guessed at or 2nd hand,
and that i'm self taught...and about to doubt a near deity...grin...
I've had a terrible time trying to forge architectural bronze...it cracks easily, has a narrow working temperature range and attempts at repair turn ugly. Machines nicely though.
Al bronze is buttery in it's temperature range, but unforgiving out of it.
Silicon bronze alloys vary, but trend to be kinda sticky, plastic and more forgiving.
The more zinc in an alloy, i found, the narrower the forging temperature range.
Also the more zinc, the less successive working heats it would tolerate, it seemed.
"Naval" bronze alloys and" everdure" i played with were quite forgeable.
I speculate that when Jim says forgeable, he is thinking in terms of rollers and presses and excellent temperature control.
For me, it's hammer , anvil, treadle hammer tooling, gas forge or torch more likely and sloppy eyeball temperature estimates.
On Feb 17, 2013, at 6:11 PM, James Binnion wrote:
Historically bronze was a copper tin alloy but also had lots of other things in it as well due to less the materials and processes available. Today a copper alloy that does not have zinc or nickel as the second significant metal in the alloy is a bronze.
The closest thing you can buy to that real bronze is what is called phosphor bronze it is 94.8% copper, 5% tin and a tiny amount .2% of phosphorous to deoxidize the metal. The trade number for this material is C5100 or C510. The stuff is tough to work and not a good choice for hot working, in fact no copper tin alloy will be a good hot work alloy.
The best forging alloy is called Architectural Bronze (C3850) which is actually a brass as it has zinc as the second greatest metal in the alloy after copper. 57% Cu, 40% Zn, 3% Pb just don't weld it as the lead makes it a poor choice for welding both from a health and performance aspect.
A reasonable compromise alloy is Commercial Bronze (C2200) which has reasonably good hot work properties and can be TIG welded but it is again a brass called bronze at 90% Cu, 10% Zn
James Binnion
jbin at well.com
______________________________________________________________
TheForge mailing list
Home: http://mailman.qth.net/mailman/listinfo/theforge
Help: http://mailman.qth.net/mmfaq.htm
Post: mailto:TheForge at mailman.qth.net
TheForge mail list group photo site is
http://www.photoworks.com
Login: blacksmithblacksmith at hotmail.com
Password: anvil
This list hosted by: http://www.qsl.net
Please help support this email list: http://www.qsl.net/donate.html
------------------------------
_______________________________________________http://mailman.qth.net/mailman/listinfo/theforge
TheForge mail list group photo site is
http://www.photoaccess.com
Login: blacksmithblacksmith at hotmail.com
Password: anvil
End of TheForge Digest, Vol 109, Issue 17
*****************************************
______________________________________________________________
TheForge mailing list
Home: http://mailman.qth.net/mailman/listinfo/theforge
Help: http://mailman.qth.net/mmfaq.htm
Post: mailto:TheForge at mailman.qth.net
TheForge mail list group photo site is
http://www.shutterfly.com
Login: blacksmithblacksmith at hotmail.com
Password: anvil
This list hosted by: http://www.qsl.net
Please help support this email list: http://www.qsl.net/donate.html
More information about the TheForge
mailing list