[TheForge] anvil repair

Bruce . freemab222 at gmail.com
Sat Apr 27 11:46:00 EDT 2013


C'mon, Frosty.  Tell us what you really think! ;^)

On Fri, Apr 26, 2013 at 2:20 PM, Jerry Frost <akfrosty at mtaonline.net> wrote:
>
> These are ALL HARDFACING rods and wire!! ARGHHHHH!!!
>
> They're abrasion resistant and really unsuitable unless you're planning on
> rubbing rocks on your anvil face.
>
> Use buildup rod or wire, it's intended to provdie an IMPACT resistant
> substrate so hardfacing won't check and spall in flexion. Buildup doesn't
> work harden, it's already impact resistant enough to take a dozer's worth of
> abuse without denting or work hardening. You can lay multiple passes without
> preheating, post heating or worrying about it. It's designed to build up and
> replace LOST steel. It grinds well with common stone cups or right angle
> disks,NOT blue or green wheels, just plain old grinding disks and cups.
>
> GET OFF THE HARDFACING KICK!  It's a myth and not only doesn't work it
> damages anvil faces with all the BADNESS of over heating HC steel faces!, It
> also causes many times the work to finish but I don't really CARE if you
> guys want to do ten times the work neccessary for a poor surface. I DO care
> about all the anvils hardfacing rod and wire are ruining!
>
> I know of which I speak, I ran hardfacing rods and wire for 20 years and had
> to clean up messes made by guys who THOUGHT harder was better. DOLTS! Yeah,
> I've run a few THOUSAND lbs. of Lincore 50 and it's superior for what it's
> intended HARD FACING, NOT anvil repair.
>
> Jer
>
>
> On 4/25/2013 5:10 PM, Andrew Vida wrote:
>>
>> Grind all broken areas until nothing but bright metal shows.  Follow
>> cracks all the way until they are no more.  Preheat anvil to 400* even if
>> manufacturer of hardface material says it is not needed. It is.
>>
>> Lay in your hardface material.  Grind to your desired geometry. Done.
>>
>> The best electrodes we (NJBA) ever used was Hobart SmoothArc 600, but that
>> does not come in wire - stick only.  For wire we used Lincore 50, though I
>> believe they have gone to Lincore 55 now and it works very well.  I prefer
>> material that goes on at full hardness.  The work hardening materials are
>> not to my liking. YMMV, of course.
>>
>> On 4/24/2013 7:14 AM, James wrote:
>>>
>>> I know this has been discussed before but I need a refresher course...
>>>
>>> Bought an old (1856) William Foster anvil a few weeks ago. The top is
>>> pretty flat but the edges are beaten off almost all the way around and a
>>> couple places that appear to have rips or tears in the top.
>>>
>>> According to the Postman book, Anvils in America it has a wrought base
>>> and a steel top that was forge welded.
>>>
>>> If you were to attempt to rebuild the corners/edges of this anvil, what
>>> procedure would you follow? And what electrodes would you use?
>>>
>>> My inclination is to clean it as much as possible, pre-heat to about400
>>> degrees F, weld the bottom of any holes that cannot be cleaned without
>>> doing serious damage to the anvil with a 6010 electrode (because it
>>> tolerates rust and junk and penetrates deeply). Then build up the
>>> surfaces with something like a 7018, grind down, etc. (I've read the
>>> 7018 works pretty well rebuilding an anvil.)
>>>
>>> I have an almost full 50# box of Lincoln Abrasoweld that I use
>>> occasionally but don't know if it's for impact, abrasion or both. I
>>> hesitate to use an extremely hard rod on an anvil. On the other hand, in
>>> the 40 years that I've been welding I've used Stoody, Hi-Alloy, Hobart,
>>> specialty rods etc. with generally good success. Those rods used to be
>>> pretty common here (100 mi. NE of Dallas, TX) but now you just about
>>> can't get any special stick rods (Ni for cast iron being and Hi-Alloy
>>> 500 the only exceptions).
>>>
>>> I presume this is due to the extreme popularity of MIG machines and the
>>> guys using portable rigs only use 6010/11 and 7018 for most work. All
>>> that to say, specialty rods are hard to find here and the boys in the
>>> welding shops aren't very helpful.
>>>
>>> Would you go to the trouble to find a different rod selection than what
>>> I have mentioned and what procedure would you recommend if different
>>> from the above? Since Postman says the body of this anvil is wrought -
>>> and I've never stick welded wrought iron - will I have any difficulties
>>> if I get down into the wrought part?
>>>
>>> And one more question, just how well would a MIG w/ standard
>>> off-the-shelf MIG wire and 92/8 or 75/25 shielding gas work to repair an
>>> anvil?
>>>
>>> Thanks,
>>> James
>
>
> ______________________________________________________________
> TheForge mailing list
> Home: http://mailman.qth.net/mailman/listinfo/theforge
> Help: http://mailman.qth.net/mmfaq.htm
> Post: mailto:TheForge at mailman.qth.net
>
> TheForge mail list group photo site is
> http://www.shutterfly.com
> Login: blacksmithblacksmith at hotmail.com
> Password: anvil
>
> This list hosted by: http://www.qsl.net
> Please help support this email list: http://www.qsl.net/donate.html



-- 
Bruce
NJ


More information about the TheForge mailing list