I think EA Chase effected the tempering step by burying 
the cutting edge in a fat piece of hot steel.

David E. Smucker wrote:
> Dave,  For this tool do the following.
> 
> Heat to a good yellow heat, around 1850 to 1900 F.
> 
> Let air cool (quench) in still air down to 140 F -- you can just touch / 
> hold it like very hot water.
> 
> Temper by heating to 1050 F.  Blood red in very low light.
> 
> Let cool and put to use.
> 
> The tempering step is important and most folks are surprised to see it this 
> high.  There is actually a secondary hardening effect that takes place with 
> the temper step.  Final hardness will be around Rockwell C of 50 to 51.
> 
> Not textbook treatment but not far off.
> 
> Dave Smucker
> Brasstown, NC
> 
> --------------------------------------------------
> From: "Dave Mudge" <dave at magichammer.net>
> Sent: Tuesday, May 25, 2010 1:25 PM
> To: "Blacksmithing List Sponsored by ABANA" <theforge at mailman.qth.net>
> Subject: [TheForge] Hardenind H-13
> 
>> Good afternoon,
>> I am looking for a SIMPLE & FAST way to harden H-13.
>> I made a special chisel type tool actually it's more of a
>> pushing tool for beveling one edge of a chisiled line.
>> The tool is about 5/8 inch round stock and 6 inches long.
>> It is for use on the treadle hammer.
>> thanks,
>> dave mudge
>> ______________________________________________________________
>> TheForge mailing list
>> Home: http://mailman.qth.net/mailman/listinfo/theforge
>> Help: http://mailman.qth.net/mmfaq.htm
>> Post: mailto:TheForge at mailman.qth.net
>>
>> TheForge mail list group photo site is
>> http://www.photoaccess.com
>> Login: blacksmithblacksmith at hotmail.com
>> Password: anvil
>>
>> This list hosted by: http://www.qsl.net
>> Please help support this email list: http://www.qsl.net/donate.html
>>
> ______________________________________________________________
> TheForge mailing list
> Home: http://mailman.qth.net/mailman/listinfo/theforge
> Help: http://mailman.qth.net/mmfaq.htm
> Post: mailto:TheForge at mailman.qth.net
> 
> TheForge mail list group photo site is
> http://www.photoaccess.com
> Login: blacksmithblacksmith at hotmail.com
> Password: anvil
> 
> This list hosted by: http://www.qsl.net
> Please help support this email list: http://www.qsl.net/donate.html
> 


More information about the TheForge mailing list