By volume, but the densiy of each of the materials is roughly the same.
Lotta air in ground up steel wool. I think anhydrous borax ground up fine
mught be a bit heavier, so I'll probably get a postage or dietary scale when
I make up a batch with anhydrous.
Actually, I didnt trash the mill at all. The steel cutters are a LOT
harder than steel wool,and grind it up w/o much pressure at all. Just
cleaned everything up good.. Course, I'll run a lot of oats through there
for the compost before I use it for food again.
----- Original Message -----
From: "Paul" <crosspein at sbcglobal.net>
To: "Sponsored by ABANA" <theforge at mailman.qth.net>
Sent: Tuesday, April 15, 2008 5:44 PM
Subject: Re: [TheForge] Re: New Discoveries: Ersatz EZ Weld
> Peter,
> How did you measure the percentages? Is this by weight or volume?
>
> While I'm not about to trash my grain mill as it still gets plenty of use
> smashing various malted grains, I'm curious about this mix and may very
> well try it.
>
> thanks,
> **paul
>
> Peter Hirst wrote:
>> Success! 60% Borax, 20% Boric Acid, 20% fine steel. Did a 6" faggot
>> weld w/ 3/8 in 3 heats. The weld stood up to a cold chisel and 4lb
>> drill hammer. Steel wool fibers were visible in the foamy part of the
>> flux, separate from the work, right up to welding heat. If I ever get a
>> hold of some wire rope for a knife, this is the flux I'll use. Next step
>> is to make anhydrous. the bubbling off of the H2O wastes a lot am flux
>> and I'm sure doesn't cover as well.
>>
>> Thanks for all the input.
>>
>> Keziah
>>
>>
> _______________________________________________
> Manage membership or unsubscribe at:
> http://mailman.qth.net/mailman/listinfo/theforge
> theforge mail list group photo site is
> http://www.photoaccess.com
> Login: blacksmithblacksmith at hotmail.com
> password: anvil
> ___________
>
>
>
More information about the TheForge
mailing list