Pot failure is mainly caused by improper fire management. Instructors
want to get people hooked on blacksmithing by having them hit hot
iron, very few take the time to teach proper fire control and management.
The wearing out of fire pots comes from letting the fire get to the
pot.. ie.. letting the fire burn down till there is insufficient fuel
left..or letting the fire burn out to the walls of the pot. There
should always be green coal in contact with the pot.. you feed the
fire from the sides ... in. In other words, push the coal down the
inside of the wall.. forcing the coke to the center.. then as the
green coal cokes.. it is pushed inwards by new coal..
Water is used to help keep the fire from spreading throughout the
pot.. I have seen pots cracked by water but that was after the fire
got out of hand and TOO much water was used. I use either a sprinkle
cup or a rag on the end of a rod to control flames.. think of it like
knocking back the hot spots when BBQing..
Ive actually forged all day, and when I took the fire apart that
night, Ive found bits of un burned newspaper from when I started the
fire that morning.
Lastly.. my fire pot IS made of stainless.. its 3/8" plate and
actually is a pot within a pot, which actually air cools the pot as
the air is blown in. Its about 10 years old now and has barely
changed color. However a good cast iron firepot should last several
lifetimes if proper fire management is practiced.
mike
At 07:11 AM 7/4/2007, you wrote:
>Hello
>Parts of this discussion have mentioned firepots "wearing out" or
>"cracking".
>I have been led to believe that the use of water on the fire as the
>cause of this destruction.
>How does water factor into the longevity or lack of the pots life?
>Thank you
>lynn
>
>_______________________________________________
>Manage membership or unsubscribe at:
>http://mailman.qth.net/mailman/listinfo/theforge
>theforge mail list group photo site is
>http://www.photoaccess.com
>Login: blacksmithblacksmith at hotmail.com
>password: anvil
>___________
Mike Linn
Artist Blacksmith
McCalla, AL
______________________________________________________________________
"Many of life's failures are people who did not realize how
close they were to success when they gave up. "
~ Thomas A. Edison
______________________________________________________________________
More information about the TheForge
mailing list