The first is that you will need a bigger furnace.  Next is that you will
need lots of flux.  And you will need a real crucible.  The melting temp of
copper is not that far off of that of steel.  Your crucible will be red hot
and fragile. A clay graphite or silicon carbide crucible is what you will
want to use.  If you are just burning off the insulation use a weed burner.

Dan in Auburn 

-----Original Message-----
From: theforge-bounces at mailman.qth.net
[mailto:theforge-bounces at mailman.qth.net] On Behalf Of Bob Willman
Sent: Thursday, June 29, 2006 4:05 PM
To: 'terry l. ridder'; 'Sponsored by ABANA'
Subject: RE: [TheForge] reclaiming copper

	Burn the insulation off in a bon-fire. 


Bob Willman
Bowling Green, Ohio
The Eagle's Anvil
WB8NQW

-----Original Message-----
From: theforge-bounces at mailman.qth.net
[mailto:theforge-bounces at mailman.qth.net] On Behalf Of terry l. ridder
Sent: Thursday, June 29, 2006 5:39 PM
To: theforge at mailman.qth.net
Subject: [TheForge] reclaiming copper

hello;

i have roughly 700 lbs of copper cable and wire. the majority of this amount
still has insulation intact. i have researched the possible ways to reclaim
the copper minus the insulation. the reason for wanting to remove the
insulation is purely economic. the local scrap dealer pays 0.05 us cents per
lbs unclean copper. $2.69 usd per lbs for clean copper.

assuming that 90 percent is copper.

so
700 * 0.05 = $35.00 usd
700 * 2.69 * 0.9 = $1694.70 usd


manual strip by hand way.
strip the insulation using wire strippers and/or utility knives.


the shred and acid way.
shredding the copper cable and wire and placing the shredded mix into
sulphuric acid.
place a copper plate cathode in the acid solution. place some of the large
copper cables in the acid solution to act as anodes.
connect a direct current power source and plate out the copper.

the shred and smelt way.
shredding the copper cable and wire and placing the shredded mix into a
crucible furnace which melts the copper and incinerates the insulation.
the problem with this method is the casting copper into anything other than
ingots is difficult.

i have two coffee can foundries and several 3 inch schedule 80 pipe
curcibles.
i was thinking of just making ingots. i have several ingot moulds made from
angle iron that i use for aluminum.

my thinking is cut the cable and wire into 6 inch long pieces. preheat these
lenghts on the crucible furnace lid than add to the crucible. after a pound
or two pour the ingots.

anyone have any suggestions comments?

anyone ever dealt with reclaiming a large amount of copper before?

--
terry l. ridder ><>
_______________________________________________
Manage membership or unsubscribe at:
http://mailman.qth.net/mailman/listinfo/theforge
theforge mail list group photo site is
http://www.photoaccess.com
Login:  blacksmithblacksmith at hotmail.com
password:  anvil
___________





_______________________________________________
Manage membership or unsubscribe at:
http://mailman.qth.net/mailman/listinfo/theforge
theforge mail list group photo site is
http://www.photoaccess.com
Login:  blacksmithblacksmith at hotmail.com
password:  anvil
___________




More information about the TheForge mailing list