[TheForge] Repairing power hammer dies

Cameron Stoker cameron at stoker.net
Sun Jun 11 08:47:03 EDT 2006


I'm afraid it was smaller than you're talking about - one side chip 
about 3/8" w x 1/8"d x 1/4 h - doing fine.  A couple other divots caused 
by a hard chisel shank 3/8" diam x 1/16 deep. Make sure to pickle or 
otherwise clean your rod/spring wire very well & degrease the die. I had 
a handful of pinholes apear when I used a wire with a little surface 
rust present.  This is just good welding practice. To get really clean 
welds you have to follow all the rules. I fudge the rules on 'hidden' 
tig tacks on ornamental pieces and this can lead to bad habbits.
	I've also thought of using small O-1 rods or w-1, but have yet to try 
this. The cooling from the large die block works just at about the right 
rate to get tough 5160 weld repair spots. There is probably a 
ring-shaped band around the weld repair that gets hot enough to temper 
further, but not hot enough to harden. In practice the whole weld repair 
is a bit softer than the parent metal, but tougher than 70xx rod repairs.

Ralph Sproul wrote:
> 	Cameron,  Thanks for this info on the die repair.  I have a chipped die and
> will try this.
> 
> 	It sure make sense that a medium carbon spring wire would lend itself to a
> tough but not to hard repair in tig welding - I see that 5160 is a
> low chrome alloy for springs.  So a tough repair with a chrome (being that
> it has good impact qualities makes a lot of sense) should be a good one
> for impact and toughness.
> 	Just curious as to your results - what is the largest repair area you've
> done on a die?  about a 1/4" square - or something 1/4 x 3/4 as like
>  a chipped edge?  Or have you filled scale abraded hollows with good success
> as well?
> 
> Thanks,
> 
> Ralph
> 
> -----Original Message-----
> From: theforge-bounces at mailman.qth.net
> [mailto:theforge-bounces at mailman.qth.net]On Behalf Of Cameron Stoker
> Sent: Wednesday, June 07, 2006 5:21 PM
> To: Sponsored by ABANA
> Subject: Re: [TheForge] Repairing power hammer dies
> 
> 
> On a set of little giant dies I've repaired chips by tig welding the
> void using an uncoiled spring (~1/8" diam wire) as filler material.
> I'd guess most springs are 5160 -ish in composition. I've had
> surprisingly little cracking of these repairs.
> 
> 
>                  Cameron Stoker
>                  cameron at stoker.net
>                  "May you run like a vicuña!"
> 
> _______________________________________________
> Manage membership or unsubscribe at:
> http://mailman.qth.net/mailman/listinfo/theforge
> theforge mail list group photo site is
> http://www.photoaccess.com
> Login:  blacksmithblacksmith at hotmail.com
> password:  anvil
> ___________
> 
> 
> 
> 
> _______________________________________________
> Manage membership or unsubscribe at:
> http://mailman.qth.net/mailman/listinfo/theforge
> theforge mail list group photo site is
> http://www.photoaccess.com
> Login:  blacksmithblacksmith at hotmail.com
> password:  anvil
> ___________
> 
> 


-- 
                 Cameron Stoker
                 cameron at stoker.net
                 "May you run like a vicuña!"


More information about the TheForge mailing list