Justin, To re temper Al after you have had your way with it is a fairly easy
process but you will need an electric furnace that will be able to hold you
work suspended on a rack. Heat to 900 deg f for one hour, ( bring up to
temp in 30 min hold for 30 min) quench in cold water, heat to 350 hold
for 12 hours. Air cool in furnace for 12 hours. This should return the
metal to around T6 temper. Before doing this on production work that your
life will depend on do a test piece.
Dan in Auburn
-----Original Message-----
From: theforge-bounces at mailman.qth.net
[mailto:theforge-bounces at mailman.qth.net] On Behalf Of Ries Niemi
Sent: Tuesday, February 14, 2006 9:11 AM
To: Sponsored by ABANA
Subject: Re: [TheForge] tempering aluminum
On Feb 14, 2006, at 6:24 AM, Justin Fellenz wrote:
> Does anyone know about how to re-temper aluminum? I know very little
> about how aluminum works beyond how to anneal it to make it soft and
> to forge when hardwood leaves a skidmark. But I was thinking about
> whether it would be possible to build a motorcycle swingarm (I'm
> thinking a swoopy single-sided job) by hammerforming a three-sided
> shape hot and then welding in internal bracing and the fourht side to
> make a box. But then it would be annealed, and I suspect that it
> should be a good springy temper. T-6 seems to be the common one.
>
> Really airing out my ignorance here, but none of my books have
> anything on this.
>
> Thanks,
>
> JRF
This is probably not feasible in a home shop type environment.
Commercially, they use big, very temperature controlled ovens,
sometimes they water quench, but the recipes are tricky, and vary with
the slightest change in alloy. Some alloys will age harden, others only
work harden.
Overbuild, internal brace, and dont worry about it getting softer.
Ries Niemi
Industrial Artist
http://www.RiesNiemi.com
_______________________________________________
Manage membership or unsubscribe at:
http://mailman.qth.net/mailman/listinfo/theforge
theforge mail list group photo site is
http://www.photoaccess.com
Login: blacksmithblacksmith at hotmail.com
password: anvil
___________
More information about the TheForge
mailing list