[TheForge] Stainless contamination
Paul Sperbeck
forge at wi.rr.com
Wed Aug 24 17:05:41 EDT 2005
I seem to have misplaced the original message on this topic, but thought
that I would point out something else that will cause 'surface rust' on
stainless steel.
If you have used a wire wheel that is carbon steel or a stainless steel
wire wheel that has been used on carbon steel, you will transfer enough
iron to the surface to cause rusting of the transfered particles. In
this case re cleaning with a stainless steel brush may not remove all
the contamination, and a pickle to remove the free iron may help.
--
Paul C. Sperbeck
My Grandfather was a blacksmith,
...and It didn't do me one damn bit of good.
Pieces of seven, pieces of seven - A parroty error.
The information in this transmission is intended to be totally worthless and devoid of any benefit to anyone with the exception of, possibly, the intended recipient. If you received this communication in error or if you accidentally read it when it wasn't addressed to you, then please immediately delete all of your saved game files and email addresses and then energetically beat yourself about the head and shoulders with a recent technology publication of your choice. All other more intelligent actions taken in response to this information are prohibited, so there.
"To err is human...to really f*** things up requires the root password."
The following added for automatic email harvesters!
abuse at worldatt.net abuse at prodigy.net abuse at bellsouth.net abuse at yahoo.com
UCE at FTC.GOV abuse at tesco.net abuse at freeserve.net
--
No virus found in this outgoing message.
Checked by AVG Anti-Virus.
Version: 7.0.344 / Virus Database: 267.10.15/81 - Release Date: 8/24/2005
More information about the TheForge
mailing list